TEST RESULTS
Absorption & Density
Sample | Absorption | Density |
---|
GOLD |
3.89 |
2.34 |
ROYAL BEIGE |
0.11 |
2.69 |
SILVER |
1.09 |
2.48 |
NOCE |
0.98 |
2.58 |
ELLA |
1.08 |
2.46 |
YOSEMITE |
1.10 |
2.49 |
WHITE CREAM |
0.80 |
2.51 |
AFYON ICE MARBLE (SB) |
0.12 |
2.71 |
BLUE MARBLE (SB) |
0.12 |
3.03 |
CREAMA WINTER (SB) |
0.22 |
2.63 |
Compressive Strength
Sample | Dry - Avg Psi |
---|
GOLD |
11,410 |
ROYAL BEIGE |
25,000 |
SILVER |
9,300 |
NOCE |
17,890 |
ELLA |
9,290 |
YOSEMITE |
9,310 |
WHITE CREAM |
18,310 |
AFYON ICE MARBLE (SB) |
14,550 |
BLUE MARBLE (SB) |
15,050 |
CREMA WINTER (SB) |
22,090 |
Resistance to Freeze Thaw
Sample | Result | Note |
---|
GOLD |
Passed |
No crack or deformation |
ROYAL BEIGE |
Passed |
No crack or deformation |
SILVER |
Passed |
No crack or deformation |
NOCE |
Passed |
No crack or deformation |
ELLA |
Passed |
No crack or deformation |
YOSEMITE |
Passed |
No crack or deformation |
WHITE CREAM |
Passed |
No crack or deformation |
AFYON ICE MARBLE (SB) |
Passed |
No crack or deformation |
BLUE MARBLE (SB) |
Passed |
No crack or deformation |
CREMA WINTER (SB) |
Passed |
No crack or deformation |
Coefficient of Friction
Sample | Dry | Wet | Result |
---|
GOLD |
1.42 |
1.16 |
Passed |
ROYAL BEIGE |
1.43 |
1.14 |
Passed |
SILVER |
1.45 |
1.15 |
Passed |
NOCE |
1.44 |
1.16 |
Passed |
ELLA |
1.45 |
1.15 |
Passed |
YOSEMITE |
1.44 |
1.16 |
Passed |
WHITE CREAM |
1.47 |
1.18 |
Passed |
AFYON ICE MARBLE (SB) |
1.02 |
0.63 |
Passed |
AFYON ICE MARBLE (SB) |
1.02 |
0.65 |
Passed |
CREMA WINTER (SB) |
0.92 |
0.52 |
Passed |